Urssa 300. High hardness steel
Soldering: Excellent
Folded: Good
Transformation: Good
Mechanization: Good
General specifications*
C 0,16-0,24. Mn 0,90-1,55. Si 0,20-0,50. P ≤ 0,035. S ≤ 0,025. Cr 0,80-1,20. Mo 0,15-0,50. Carbono equivalente 0,65.
Rm800/1.000 N/mm2. ReH≤ 550 N/mm2. A ≥ 14 %. Dureza Brinell 280/350 Hb. Factor antidesgaste60.
TYPICAL APPLICATION
Production of pieces that require a good performance to abrasion and at the same time a good toughness. Like pots, high density blades, demolition clamps, pieces and plates for O.P equipment, etc.
SOLDERING
It can be sold using the traditional system.
It is recommended to use dry metal flow adequate with the controlled hydrogen.
It is recommended to preheat the soldering zone, use Hilo Autrod 13-29 OK, basic Fluxocord 42/0841 TT Orlikon electrode or similar.
SHAPING
Warm way: should be hot forming and It is recommended to upright in the sense of lamination.
MECHANIZATION AND OXYCUT
Good. Anneal or stabilized following oxycut recommended.
Thermal processes
Treatment | Temperature | Refrigeration |
---|---|---|
Preheating | 670 – 700 ºC | Oven |
Cementation | 900 – 950 ºC | Oil, air, salts |
Normalize | 860 – 880 ºC | Air |
Warm up | 860 – 880 ºC | Oil or salts 200ºC |
810 – 830 ºC | Oil or water | |
Drawn Stainless | 150 – 200 ºC | Air |
* To mechanize easily your pieces, ask for our stabilized heat softening treatment.
Stock Program
* The specifications are illustrative. For each supply we offer a certificate with the datum of the shipment delivered.